超碰人人看人人射-五月婷婷青青综合啪啪-99精产国品一二三产-久久fc2亚洲-精品人妻互换一区二区三区-日韩国产v片一区二区三区免费看-蜜臀99久久精品久久久懂爱-麻豆成人在线免费观看视频-久久九九视频在线观看,伊人久久婷婷亚洲,人妻系列中文字幕大全,日韩久久久久久蜜臀av

產(chǎn)品展示
當(dāng)前位置:首頁(yè) > 全部產(chǎn)品 > 英國(guó)Ossila > 材料 > Ossila材料PTB7 CAS:1266549-31-8 PTB7

Ossila材料PTB7 CAS:1266549-31-8 PTB7

Ossila材料PTB7 CAS:1266549-31-8 PTB7
Ossila代理、*、交期準(zhǔn)時(shí)、歡迎新老客戶?。。?/p>

分享到:

只用于動(dòng)物實(shí)驗(yàn)研究等

Batch Information

Batch No.MwPDStock Info
M21118,0001.75Sold out
M212> 40,0002.0Sold out
M21385,0002.0In stock

Ossila材料PTB7 CAS:1266549-31-8 PTB7

Applications

PTB7 for high-performance organic photovoltaics.

Poly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]], more commonly known as PTB7.

In stock now for immediate dispatch worldwide.

PTB7 gives some of the highest reported efficiencies for polymer:fullerene solar cells due to its extended absorption into the near infra-red and lower HOMO level. Together with our complete package of processing information, PTB7 becomes a quick and easy way to improve device efficiencies. This represents a cost-effective method to increase performance and impact of devices and data for a wide range of OPV related research.

At typical concentrations for spin-coated devices of 10 mg/ml, a standard batch of 100 mg will produce 10 ml of ink - enough to coat 200 of Ossila's standard sized substrates even assuming 50% ink loss during preparation and filtration. At concentrations of 1 mg/ml (more typical for ink-jet printing and spray coating) up to 100 ml of ink can be produced.

In a standardised reference architecture (using a PEDOT:PSS hole interface and Ca/Al electron interface) we have shown this batch to give a PCE of 6.8% (see data sheet below) and up to 7.4% using PFN. By using new interface materials and architectures PTB7 has been shown to reach efficiencies of 9.2% PCE in the literature [1,2].

The high solubility in a wide range of solvents makes ink preparation and filtration simple, and PTB7 is one of the easiest materials we have ever worked with (simply shake it to dissolve). This also makes it an excellent candidate for a variety of coating techniques including ink-jet printing, spray coating and blade coating.

For information on processing please see our specific fabrication details for PTB7, general fabrication video, general fabrication guide, optical modelling paper on our standard architecture [3], or us for any additional help and support.

References (please note that Ossila has no formal connection to any of the authors or institutions in these references):

  • [1] Enhanced power-conversion efficiency in polymer solar cells using an inverted device structure Zhicai He et al., Nature Photonics, V 6, p591–595 (2012).
  • [2] Simultaneous Enhancement of Open-Circuit Voltage, Short-Circuit Current Density, and Fill Factor in Polymer Solar Cells Zhicai He et al., Advanced Materials, V 23, p4636–4643 (2011).
  • [3] Optimising the efficiency of carbazole co-polymer solar-cells by control over the metal cathode electrode Darren C. Watters et al., Organic Electronics, V 13, p1401–1408 (2012)
  • [4] Designing ternary blend bulk heterojunction solar cells with reduced carrier recombination and a fill factor of 77%, N. Gasparini et al, Nat. Energy, 16118 (2016); doi:10.1038/nenergy.2016.118 (Ossila PTB7 was featured in this paper).

Ossila材料PTB7 CAS:1266549-31-8 PTB7

Datasheet

PTB7 chemical structureChemical structure of PTB7; Chemical formula (C41H53FO4S4)n.

Specifications

Full namePoly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]]
SynonymsPTB7
CAS number1266549-31-8
Absorption670 nm (CH2Cl2), 682 nm (film)
SolubilityChloroform, Chlorobenzene, o-DCB

 

Usage Details

Inverted Reference Devices

Reference device were made on batch M211 to assess the effect of PTB7:PC70BM active layer thickness on OPV efficiency using an inverted architecture with the below structure. These consisted of the below structure and were fabricated under inert atmosphere (glovebox) before encapsulation and measurement under ambient conditions.

Glass / ITO (100 nm) / PFN (6.5 nm) / PTB7:PC70BM (1:1.5) / MoOx (15 nm) / Al (100 nm)

For generic details please see the general fabrication guide and video. For specific details please see the below condensed fabrication report which details the optical modelling and optimisation of the multilayer stack.

Previously it has been shown that PFN of around 6.5 nm gives optimum performance [1-3,P021] while modelling has shown that an Al back cathode gives higher performance than Ag when used with MoOx [4].

The PTB7:PC70BM solution was made in chlorobenzene at 25 mg/ml before being diluted with 3% diiodooctane (DIO) to promote the correct morphology.

Active layer thicknesses of 75 nm, 90 nm and 105 nm were chosen corresponding to the lower, middle and upper end of the "thin film" absorption peak of a typical stack as predicted by optical modelling [1]. For each of these thickness a total of four substrates was produced, each with 4 pixels and the data presented below represents a non-subjective (no human intervention) analysis of the best 75% of pixels by PCE (12 pixels for each condition).

An additional two substrates were also prepared with a methanol wash to help remove the DIO as has been reported in the literature to help improve performance[5].

Overall, the maximum efficiency of 7.2% average PCE (7.4% maximum) was found at 75 nm film thickness.

 

Efficiency for different PTB7 spin speeds - inverted architectureJsc for different PTB7 spin speeds - inverted architectureVoc for different PTB7 spin speeds - inverted architecture Fill factor for different PTB7 spin speeds - inverted architectureFigure 1: PCE, Jsc, Voc and FF for inverted architecture devices at different spin speeds. Data shown is averaged with max and min overlaid with filled circles (please see note of Dektak measurements). As previously reported [1,2,3], films of approximay 90 nm give the highest performance with greater Jsc and only minor loss in fill factor.

 

PTB7 JV Curve for inverted architecture
Figure 2: The JV curve for the best performing device - inverted architecture.

 

Note 1: Dektak Thickness calibration

We normally calibrate thin films by use of a Dektak surface profiler, however the use of DIO results in an enhanced level of uncertainty in the film as the DIO will take several hours to fully dry under normal conditions and is likely to undergo some slight further shrinkage when placed in vacuum. The DIO can also be removed by baking the substrate on the hotplate at 80°C for about 10 mins which can be useful for doing quick measurements but also drives excess phase separation between the polymer and PCBM making it unsuitable for device work.

Note 2: Effect of epoxy

Due to the very high solubility of the PTB7 it was noted during fabrication that the film changed colour when in contact with the EE1 encapsulation epoxy in liquid form for extended periods indicating that there was some miscibility. Inspection of the active areas underneath the top cathode indicated that the epoxy had not seeped into the active area before curing and device metrics indicate that this did not appear to affect performance. However, we would recommend minimising contact time between the epoxy and PTB7 films before UV curing.

 

Fabrication

Substrates and cleaning

  • Pixelated Cathode substrates (S173)
  • 5 mins sonication in hot Hellmanex III(1 ml in beaker)
  • 2x boiling water dump rinses
  • 5 mins sonication in warm IPA
  • 2x dump rinses
  • 5 mins sonication in hot NaOH
  • Dump rinse in boiling water
  • Dump rinse in water
  • Stored in DI water overnight and until use

PFN Solution

  • Dissolved at 2 mg/ml
  • Acetic acid dissolved 1:9 in methanol to make stock solution
  • 2 μl/ml of acetic added to solution
  • Stirred for 30 mins
  • Filtered through 0.45 μm PVDF filter

PFN Test Films

  • PFN Test film initially spun at 500 rpm and gave 20 nm
  • Second test film spun at 1000 rpm and gave 16 nm
  • Thickness was extrapolated to 6.5 nm at 6000 rpm

Active Layer Solution

  • Fresh stock solutions of PTB7 (Ossila M211) made on at 10 mg/ml in CB and dissolved with stirbar for 1 hour
  • Mixed 1:1.5 with dry Ossila 99% C70 PCBM to make overall concentration of 25 mg/ml and dissolved with stirbar for 1 hour
  • Old stock solution of 1,8 Diiodooctane mixed 1:1 with CB to make measuring out small quantities easier
  • DIO/CB mixture added to solution to give overall DIO amount of 3%

Active Layer Test Films

  • Test film spun at 1000 rpm for 2 mins using unfiltered solution and dried using methanol before Dektak
  • 1000 rpm gave approximay 85 nm

Active layers

  • Devices spun using 30 μl dynamic dispense (20 μl gave only moderate wetting/coverage)
  • Non methanol devices spun for 2 mins
  • Methanol devices spun for 30 seconds, then coated with 50 μl methanol by static dispense then spun at 2000 rpm for 30 seconds.
  • Cathode wiped with CB
  • Vacuum dried in glovebox antichamber for 20 mins

Evaporation

Left in chamber over the weekend and evaporated with the below parameters.

  • 15 nm MoOx at 0.2 ?/s
  • 100 nm Al at 1.5 ?/s
  • Deposition pressure

Encapsulation

  • As standard using Ossila EE1, 30 mins UV in MEGA LV101

Measurements

  • JV sweeps taken with Keithley 237 source-meter
  • Illumination by Newport Oriel 9225-1000 solar simulator with 100 mW/cm2 AM1.5 output
  • NREL certified silicon reference cell used to calibrate
  • Lamp current: 7.8 A
  • Solar output at start of testing: 1.00 suns at 25°C
  • Solar output at end of testing: 1.00 suns at 25°C
  • Air cooled substrates
  • Room temperature at start of testing: 25°C
  • Room temperature at end of testing: 25°C
  • Calibrated aperture mask of size 0.256 mm2

 

Standard (Non-inverted) Reference Devices

Reference device were made on batch M211 using a standardised architecture for comparative measurements using Ossila standard substrates and materials. These consisted of the below structure and were fabricated under inert atmosphere (glovebox) before encapsulation and measurement under ambient conditions.

Glass / ITO (100 nm) / PEDOT:PSS (30 nm) / PTB7:PC70BM (variable) / Ca (2.5 nm) / Al (100 nm)

For generic details please see the fabrication guide and video. For specific details please see the below condensed fabrication report and also Watters et al. [3] which details the optical modelling and optimisation of the multilayer stack.

For this standard reference architecture an average PCE of 6.6% was achieved for the optimised thickness with a peak efficiency of 6.8%. Note that no other optimisation was performed (blend ratio, DIO concentration, drying conditions etc) and so further small improvements may be obtained by varying these conditions and significant improvements obtained by using alternative interface materials [1,2].

Efficiency for different PTB7 spin speeds - Standard architecture Jsc for different PTB7 spin speeds - Standard architecture Voc for different PTB7 spin speeds - Standard architecture Fill factor for different PTB7 spin speeds - Standard architectureFigure 3: PCE, Jsc, Voc and FF for standard architecture devices at different spin speeds. Data shown is averaged with max and min overlaid with filled circles (please see note of Dektak measurements). As previously reported [1,2,3], films of approximay 90 nm give the highest performance with greater Jsc and only minor loss in fill factor.

 

PTB7 JV curve for standard architecture
Figure 4: The JV curve for the best performing device - standard architecture.

 

Note 1: Dektak Thickness calibration

We normally calibrate thin films by use of a Dektak surface profiler, however the use of DIO results in an enhanced level of uncertainty in the film as the DIO will take several hours to fully dry under normal conditions and is likely to undergo some slight further shrinkage when placed in vacuum. The DIO can also be removed by baking the substrate on the hotplate at 80°C for about 10 mins which can be useful for doing quick measurements but also drives excess phase separation between the polymer and PCBM making it unsuitable for device work.

Note 2: Effect of epoxy

Due to the very high solubility of the PTB7 it was noted during fabrication that the film changed colour when in contact with the EE1 encapsulation epoxy in liquid form for extended periods indicating that there was some miscibility. Inspection of the active areas underneath the top cathode indicated that the epoxy had not seeped into the active area before curing and device metrics indicate that this did not appear to affect performance. However, we would recommend minimising contact time between the epoxy and PTB7 films before UV curing.

 

Fabrication

Substrates and cleaning

  • Pixelated Cathode substrates (S173)
  • 5 mins sonication in hot Hellmanex (1 ml in beaker)
  • 2x boiling water dump rinses
  • 5 mins sonication in warm IPA
  • 2x dump rinses
  • 5 mins sonication in hot NaOH
  • Dump rinse in boiling water
  • Dump rinse in water
  • Stored in DI water overnight and until use

PEDOT:PSS layer preparation

  • Clevios AI 4083
  • Filtered into vial using Whatman 0.45 μm PVDF filter
  • Spun 6000 rpm for 30 seconds (30 nm)
  • Dynamic dispense of 20 μl using pipettor
  • IPA cathode strip wipe and labelled
  • Put straight onto hotplate at 160°C as soon as cathode wiped and labelled
  • Transferred to glovebox when all samples spun.
  • Baked in glovebox at 150°C for 1 hour

Active layer Solution Preparation

  • Fresh stock solutions of PTB7 at 10 mg/ml in CB and shaken to dissolve
  • Mixed 1:1.5 with dry Ossila 99% C70 PCBM to make overall concentration of 25 mg/ml
  • 1,8 Diiodooctane mixed 1:1 with CB to make measuring out small quantities easier
  • DIO/CB mixture added to solution to give overall DIO amount of 3%

Active layer spin casting

  • Devices spun for 2 mins using 25 μl dynamic dispense
  • Cathode wiped with chlorobenzene
  • Left to dry in glovebox for 2 hours but colour indicated they were still slightly wet
  • Dried in vacuum in glovebox antichamber for 10 mins to remove DIO

Evaporation

Left in chamber over the weekend and evaporated with the below parameters.

MaterialCa
Base pressure8.0 E-8 mbar
Dep start pressure1.7 E-7 mbar
Max pressure2.7 E-7 mbar
Thickness2.5 nm
Rate0.2 ?/s
MaterialAl
Base pressure7.0 E-8 mbar
Dep start pressure6.0 E-7 mbar
Max pressure7.0 E-7 mbar
Thickness100 nm
Rate1.0 ?/s

 Encapsulation

  • As standard using Ossila EE1, 30 mins UV in MEGA LV101

Measurements

  • JV sweeps taken with Keithley 237 source-meter
  • Illumination by Newport Oriel 9225-1000 solar simulator with 100 mW/cm2 AM1.5 output
  • NREL certified silicon reference cell used to calibrate
  • Lamp current: 7.8 A
  • Solar output at start of testing: 0.99 suns at 25°C
  • Solar output at end of testing: 1.00 suns at 25°C
  • Air cooled substrates
  • Room temperature at start of testing: 21°C
  • Room temperature at end of testing: 21°C
  • Calibrated aperture mask of size 0.256 mm2

 

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細(xì)地址:

  • 補(bǔ)充說(shuō)明:

  • 驗(yàn)證碼:

    請(qǐng)輸入計(jì)算結(jié)果(填寫(xiě)阿拉伯?dāng)?shù)字),如:三加四=7

深圳市澤拓生物科技有限公司是國(guó)內(nèi)專業(yè)的Ossila材料PTB7 CAS:1266549-31-8 PTB7廠家,歡迎廣大顧客來(lái)電咨詢!
深圳市澤拓生物科技有限公司版權(quán)所有   |   技術(shù)支持:化工儀器網(wǎng)
聯(lián)系電話:0755-23003036   傳真:0755-23003036-807 GoogleSitemap 備案號(hào):粵ICP備17105262號(hào)  管理登陸
在線客服
用心服務(wù)成就你我
老头大战三个农妇对白Av-中文字幕日韩片无码 日韩中文AV-正在播放熟妇大叫受不了-四虎影视精品 | 久久好色-美女下体打码-精品无码αv一区二区三区-国产人成高清在线视频99最全资源 DVD超清免费观看 | 男女69play网站-骚穴影视大全-高清版完整版未删减 日韩欧美精品视频一区在线-少罗美女干屄漫画视频 | 婷婷久久综合九色综合97-久久78黑白配-最近国语在线观看 2878 2824 综合精品 亚洲精品无码一区二区aⅴ-中村知惠 影音先锋 | 久久 国产 小便 尿 嘘嘘-美女自慰网站免费看-少妇大叫太大太粗太爽了A片软件-蜜乳av红桃 嫩久久 | 成人一区二区三区无码-中文字幕99精品人妻少妇-成人免费国产欧美日韩你懂的-男生女生操逼国产激情AV刺激 | hdi99-成人国产自慰-竹菊传媒一区二区三区-天天干夜夜操 | 高清在线观看-亚洲国产成人久久精品影视-欧亚大尺度1区2区毛片骚逼-www7788老熟女 | 黄网WW N-国产成人自拍偷拍在线-色小姐这里全是精品-xxxxx8黄色 动漫美女老师自慰-日B视屏-国产精品无码ThePorn-一级美女日逼视频 | 国产在线观看免费播放电视剧美女图片-一区二区三区中文字幕脱狱者-91色久-gogogo高清免费观看完整版 | 国产午夜福利不卡在线观看-肏屄我要一二三区-国产成人www.-亚洲国产另类精品 | 精品人妻久久久久一区二区三区-XXXX69HD—HDm-人妻胸大逼紧靠逼视频-成年女人晚上看的干逼的一级黄色大毛片 | 嗯∽啊~轻点禁 揉胸视频在线看-巨型怪物h粗暴3d-加勒比无码北条麻妃-伊人大香蕉在线观看 | 一区二区无码在线-粉色视频在线观看完整版高清免费-美女逼中出-搜查官媚药中出一区二区 | 日韩欧美中文在线精品免费福利专区视频-久久久亚洲人妻色情-www.四虎日本-久久欧亚综合网 | 黑森林毛茸茸熟女人妻-女人自慰网址-精品国产无套在线观看-日本睡熟迷奷系列A片 | 社长秘书中出一乃葵-国产两位熟妇疯狂4p-欧美性爱去干网凝-肛交母狗双洞齐开少妇 | 国内自拍偷拍网站-DVD在线观看 亚洲欧美在线精品一区二区-国产靠逼大全-超清免费电视剧 久久精品国产亚洲?v久 | 午夜理伦精品一区二区三区在线成人-┅┅用力┅┅老熟女-国产精品三上悠亚在线观看网站-东北电影免费老师无码黄色片视屏网站大全 亚洲美女自慰-七十路熟女视频-日韩小穴-色女人综合 | 男人操东北女人对白真人视频-老熟女偷窥-欧美肥婆性猛交XXXX节目分类-国产操女人 | 国产女人逼-有坂深雪在线XX99AV-优优色综合视频-gogogo高清免费完整版如果 | 黄色片操逼-日韩欧美40路视屏-少妇人妻偷人精品免费视频-污污的网站 | 国产一级站17c-卡,99久久精品免费观看国产欧美日韩乱国产无遮挡-四虎4545www精品视频-嗯∽啊~轻点禁 揉胸视频网站观看- | 久久 国产 小便 尿 嘘嘘-美女自慰网站免费看-少妇大叫太大太粗太爽了A片软件-蜜乳av红桃 嫩久久 | 久久久永久久久人妻精品麻豆-天堂狼干伊人-天天摸夜夜添添到高潮水汪汪-国产成人一区二区在线 亚洲国产综合无码一区 | 蜜美杏中字HD在线观看-欧美美女被猛插内射的软件-久久综合桃花网中文字幕-性少妇厨房BBwBBwBBw | 亚洲国产精品一区二区不卡-91PORNY九色91肥臀-jizzjizz视频在线观看-夜色电影院 | 黄色激情成人-搡老女的BB视频-中国XXX1级黄片免费看看-丝袜试穿亚洲一区二区三区在线 | BD迅雷电影在线 菠萝菠萝蜜视频免费1-免费看大美女大奶子裸体的网站-欧美一区二区三区视频-国产亲子乱婬一级A片 | 熟女人妻去干网-骚色妞干网免费视频-情色视屏-两男一女做爱视频在线观看 | 依依狼人日日-欧美顶级黃色大片免费-720高清视频播放 日本丰满熟妇人妻av无码区-亚洲三级黄色 三区无码 | 亚洲av无码男人的天堂在线-强行中出丝袜熟女人妻-欧美精品亚洲精品日韩专区-日韩中出网 无码人妻AⅤ一区二区三区A片一 | 美女h在线观看-友田真希国产AV一九区-禁忌乱子伦-7777大胆裸体美女艺术 | 初撮り五十路の豊満女在线观看-中文字幕――色哟哟-国产精品自拍电影-密桃av. | 91麻豆糖心vlog出品淑怡熟女亚洲一区精品久久-国产精品一区无码专区-欧美V亚洲V日韩v国产Vv∨-日韩精品久久久久久久电影99爱 | 超清免费全集观看 欧洲无码的免费的毛片视频-成年女性自慰裸体网站-凤间由美Av有码中文字幕-日本少妇BB好色淫 | freevido国产-导航色一二三三网-狼人大香蕉99-国产女主播精品大秀系列 | 久久综合色之久久综合-KTV做爰视频一区二区-探花HD精品-国产午夜精品理论片久久 | 国产专区第二页-国产69精品久久久久9999apgf-色一情一乱一伦 -大胆人妻21p | 日韩欧美中文在线精品免费福利专区视频-久久久亚洲人妻色情-www.四虎日本-久久欧亚综合网 | 欧美色图11p-猛草小穴视频-少妇4p-jizzjizz草莓草莓 |