只用于動物實驗研究等

I101 perovskite Ink has been specially formulated in the Ossila laboratories to be deposited by spin coating. Our I101 perovskite ink is designed for air processing in low-humidity environments. Using a mixture of methyl ammonium iodide (MAI) and lead chloride (PbCl) dissolved in dimethyl formamide our I101 perovskite ink will convert to a methylammonium lead halide perovskite under heat. The final product is a methylammonium lead iodide perovskite with trace amounts of chlorine given by the formula CH3NH3PbI3-xClx. For information on the various applications of the mixed halide CH3NH3PbI3-xClx perovskite see our applications section.

The main use of CH3NH3PbI3-xClx is in the fabrication of solar cells, our I101 ink can be used in both standard and inverted architectures; and can achieve power conversion efficiency (PCE) values of over 13% (see our device performance section for more information). The ink specifications can be found below along with complete guides on the processing of perovskite inks for standard architecture and inverted architectures. Using our I101 recipe provided, 5ml of solution is capable of processing up to 160 substrates (1,280 devices using our 8-pixel substrate design).

 

Perovskite Ink

I101 is packaged as 10 individual vials containing 0.5 ml of solution capable of coating up to 160 substrates. I101 can also be bought in bulk (30 ml) with a 25% discount over our standard order sizes.

 

Specifications

 

Perovskite Type

CH3NH3PbI3-xClx

Precursor Materials

Methyl Ammonium Iodide (99.9%), Lead Chloride (99.999%)

Precursor Ratio

3:1

Solvent

Dimethyl Formamide (99.8%)

Optical Bandgap

1.56-1.59eV

Energy Levels

Valence Band Minimum 5.4eV, Conduction Band Minimum 3.9eV

Emission Peak

770-780nm (PL); 755-770nm (EL)

Standard Architecture PCE

13.7% Peak; 13.0% ±0.25% Average

Inverted Architecture PCE

13.1% Peak; 11.9% ±0.50% Average

Processing Conditions

Air processing; low humidity (20% to 35%)

Packaging

10x 0.5ml sealed amber vials; 3 x 10ml sealed amber vials

 

I101 Perovskite Applications

Perovskite Photovoltaics

The single biggest application of perovskite materials is for photovoltaic devices; perovskites fabricated from MAI:PbCl precursors have been used in several papers to achieve high power conversion efficiencies. The advantage of using MAI:PbCl as precursor materials is the ability to process in an ambient environment.

References

  • Efficient hybrid solar cells based on meso-superstructured organometal halide perovskites. J. Snaith et. al. Science. 338 (2012) 643-647 DOI: 10.1126/science.1228604
  • Additive enhanced crystallization of solution-processed perovskite for highly efficient planar- heterojunction solar cells. K-Y. Jen et. al. Adv. Mater. 26 (2014) 3748-3754 DOI: 10.1002/adma.201400231
  • Morphological control for high performance, solution-processed planar heterojunction perovskite solar cells. J. Snaith et. al. 24 (2014) 151-157 DOI: 10.1002/adfm.201302090

 

Perovskite LED and Lasing

Due to the high photoluminescence quantum yield of perovskites at room temperature, the application of these materials in light-emitting diodes (LEDs) is of great interest. Devices made using MAI:PbCl precursors show strong emission in the near-infrared region at 755nm. Additionally, recent work has shown lasing within this material.

References

  • Bright light-emitting diodes based on organometal halide perovskite. R. H. Friend et. al. Nature Nanotechnology, 9 (2014) 687-692 doi:10.1038/nnano.2014.149
  • Interfacial control towards efficient and low-voltage perovskite light-emitting diodes. Hang et. al. Adv. Mater. 27 (2015) 2311-2316 DOI: 10.1002/adma.201405217
  • High photoluminescence efficiency and optically pumped lasing in solution-processed mixed halide perovskite semiconductors. H. Friend et. al. J. Phys. Chem. Lett. 5 (2014)1421-1426 DOI: 10.1021/jz5005285

 

Scale-Up Processing

Due to the ability to process perovskites based upon MAI:PbCl precursors in air, the material opens up the possibility of applications in large-scale deposition techniques. Several different scalable techniques, such as slot-die coating and spray coating have been used to deposit this material.

References

  • Upscaling of perovskite solar cells: Fully ambient roll processing of flexible perovskite solar cells with printed back electrodes. C. Krebs et. al. Adv. Energy Mater. 5 (2015) 1500569 DOI: 10.1002/aenm.201500569
  • Highly efficient, felixble, indium-free perovskite solar cells employing metallic substrates, M. Watson et. al. J. Mater. Chem. A, 3 (2015) 9141-9145 DOI: 10.1039/C5TA01755F
  • Efficient planar heterojunction mixed-halide perovskite solar cells deposited via spray-deposition. G. Lidzey et. al. Energy Environ. Sci. 7 (2014) 2944-2950 DOI: 10.1039/C4EE01546K

 

I101 Perovskite Processing Guides

Standard Architecture:

FTO/TiO2(Compact)/TiO2(Mesoporous)/I101/Spiro-OMeTAD/Au

Below is a condensed summary of our fabrication routine for standard architecture devices using our I101 ink.

 

  1. FTO etching:
  • A complete guide to FTO etching can be found on our FTO product page along with an instructional video
  1. Substrate cleaning:
  • Sonicate FTO for 5 minutes in hot (70°C) DI water with the addition of 1% Hellmanex
  • Dump-rinse twice in boiling DI water
  • Sonicate FTO for 5 minutes in Isopropyl alcohol
  • Dump-rinse twice in boiling DI water
  • Dry FTO using filtered compressed gas
  • Place the FTO into the UV Ozone Cleaner and leave for 10 minutes
  1. Compact TiO2 deposition:
  • Prepare a solution of titanium diisopropoxide bis(acetylacetonate) at a volumetric percentage of 8% in isopropyl alcohol (approximay 20ml will be needed)
  • Mask off the substrates such that only the active area of the devices are exposed
  • Place the substrates onto a hotplate set to 450°C
  • Using a nitrogen/compressed air gun set it to a pressure of 16-18 psi and spray the solution onto the substrates. Leave the solution for 30 seconds to dry, and sinter and repeat the spray process again. Repeat this until you get approximay 40 nm of film, this should take around 10 sprays
  • Cover the substrates loosely with foil and leave to sinter for 30 minutes
  • After sintering remove the substrates from the hotplate, care should be taken as rapid cooling can shatter the substrate
  1. Mesoporous TiO2 deposition:
  • Using a mesoporous paste with a particle size of 18nm and pore size of 30nm, prepare a mesoporous film of approximay 200 nm thick
  • Place the substrates back on the hotplate, loosely cover with foil and sinter the substrates at 450°C for 1 hour
  • After sintering remove the substrates from the hotplate, care should be taken as rapid cooling can shatter the substrate
  1. Perovskite deposition (in air):
  • Heat I101 ink for at least 2 hours at 70°C to allow for complete redissolution of solutes
  • Allow I101 ink to cool to room temperature before deposition
  • Set the hotplate temperature to 90°C
  • Static spin coating: place substrate into spin coater, dispense 30-50 μl and start spinning at 2000 rpm for 30 s
  • Place substrate onto the hotplate and anneal for 120 minutes
  • After all FTO substrates are coated, reduce the hotplate temperature to 90°C
  • After annealing, transfer the substrates into a glovebox environment.
  1. Spiro-OMeTAD deposition (in air):
  • Prepare the following solutions; Spiro-OMeTAD at a concentration of 97 mg/ml in chlorobenzene, Li-TFSI at a concentration of 175 mg/ml in acetonitrile, and TBP at a volumetric percentage of 46.6% in acetonitrile
  • Combine 1000 μl Spiro-OMeTAD, 30.2 μl Li-TFSI, and 9.7 μl TBP solutions
  • Dispense 50 µl of the combined solution onto the perovskite, allowing it to spread across the substrate
  • Spin at 2000 rpm for 30 seconds
  • Use a high-precision mirco cleaning swab soaked in chlorobenzene to wipe the cathode strip clean
  1. Spiro-OMeTAD oxidation and anode deposition:
  • Place the substrates inside a desiccator in air and leave the substrates for 12 hours in the dark to allow for oxidation of the spiro-OMeTAD film (The amount of time required for complete oxidation of the spiro-OMeTAD may vary depending upon thickness and environmental conditions. Additional oxidation steps may be needed after deposition of anode)
  • Using thermal evaporation, deposit an 80 nm layer of gold through a shadow mask to define an active area for your device
  • Devices do not need to be encapsulated for measuring performance
  • If encapsulation is desired, the spiro-OMeTAD should be allowed to fully oxidise again before substrates are transferred into the glovebox and encapsulated

Inverted Architecture:

ITO/PEDOT:PSS/I101/PC70BM/Ca/Al

For a complete step-by-step guide please see our full perovskite solar cells fabrication guide or our instructional video guide below.

Below is a condensed summary of our routine, which is also available to download as a PDF to enable you to print and laminate for use in the clean room.

 

  1. Substrate cleaning:
  • See substrate cleaning section of standard architecture device guide
  1. PEDOT:PSS deposition:
  • Filter PEDOT:PSS using a 0.45 µm PVDF filter
  • Dispense 35 µl of the filtered PEDOT:PSS solution onto ITO spinning at 6000 rpm for 30s
  • Place substrate onto a hotplate at 120°C
  • After all ITO substrates are coated, reduce the hotplate temperature to 90°C
  1. Perovskite deposition (in air):
  • Heat I101 ink for at least 2 hours at 70°C to allow for complete re-dissolution of solutes
  • Transfer heated substrate onto spin coater, start spinning at 4000 rpm and dispense 30 μl of I101 ink and leave to spin for 30 s
  • Place substrate back onto the hotplate at 90°C for 120 minutes
  • After all ITO substrates are coated, reduce the hotplate temperature to 90°C
  • After annealing transfer the substrates into a glovebox environment.
  1. PC70BM deposition (in nitrogen glovebox):
  • Prepare a solution of PC70BM at 50 mg/ml in chlorobenzene and stir for 3 to 5 hours
  • Transfer perovskite-coated substrates into the glovebox
  • Dispense 20 µl of PC70BM solution onto the spinning substrate at 1000 rpm and spin for 30s
  • Use a micro-precision cleaning swab soaked in chlorobenzene to wipe the cathode strip clean
  1. Cathode deposition:
  • Using thermal evaporation, sequentially deposit 5 nm of calcium and 100 nm of aluminium through a shadow mask to define an active area for your device
  • Encapsulate devices using a glass coverslip and encapsulation epoxy
  • Expose to UV radiation (350 nm) for ~5 minutes (times vary depending upon source intensity) to set the epoxy

 

Wistia video thumbnail - Guide to make efficient air processed perovskite devices

 

Full length fabrication guide detailing all steps necessary for the fabrication and measurement of perovskite solar cells using Ossila I101 Perovskite Precursor Ink.

 

I101 Device Performance

Below is information on photovoltaic devices fabricated using our standard architecture and inverted architecture recipes for I101 inks. All scans were taken after 10 minutes under illumination of an AM1.5 source, using a voltage sweep from -1.2 V to 1.2 V then from 1.2 V to -1.2 V at a rate of 0.2 V.s-1; no bias soaking was performed on devices.

ArchitectureStandardInverted
Sweep DirectionForwardReverseForwardReverse
Power Conversion Efficiency (%)13.513.712.413.1
Short Circuit Current (mA.cm-2)-20.8-20.8-18.8-18.8
Open Circuit Voltage (V)0.880.900.960.96
Fill Factor (%)73736972

 

I101 standard and inverted architecture perovskite solar celll iv curvesJV curve under AM1.5 irradiation for a standard (left, courtesy of Michael Stringer-Wong, University of Sheffield) and inverted (right, courtesy of Alex Barrows, University of Sheffield) device based on Ossila's I101 ink. Device characteristics were recorded on a reverse sweep.

 

想了解更詳細(xì)的產(chǎn)品信息,填寫下表直接與我們聯(lián)系:

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細(xì)地址:

  • 補(bǔ)充說明:

  • 驗證碼:

    請輸入計算結(jié)果(填寫阿拉伯?dāng)?shù)字),如:三加四=7
深圳市澤拓生物科技有限公司 專業(yè)提供:大小鼠解剖器械包,瑞士Sipel真空泵,美國EMS電鏡耗材
深圳市澤拓生物科技有限公司版權(quán)所有   |   技術(shù)支持:化工儀器網(wǎng)
聯(lián)系電話:0755-23003036   傳真:0755-23003036-807 GoogleSitemap 備案號:粵ICP備17105262號  管理登陸
在線客服
紧缚sm国模视频一区二区三区-久久国产午夜精品理论片应用-搡BBBB搡BBB搡五十-国产又色又爽又黄在线观看视频 | 精品人妻久久久久一区二区三区-XXXX69HD—HDm-人妻胸大逼紧靠逼视频-成年女人晚上看的干逼的一级黄色大毛片 | 最好的迅雷电影下载网,分享最新电影,高清电影、综艺、动漫、电视剧等下载!-丝袜av在线丝袜av天堂国产-日本少妇ⅩXXX无码妖精视频-DVD高清完整版播放 日韩欧美精品一区二区三区在线 | 黑丝美女被c在线观看-亚洲中文字幕在线观看-中文字幕一区二区三区夫目前犯-中文字幕日韩专区下载 九九99热久久10精品 | 久久久久久久久久久久久国产-中曰韩操逼大毛片基地-英国视频一级AAAAA网站-高清电影-免费完整版 国产成人一区二区三区视频免费 欧–美–性–交–黄–片-淫辱列车员(全黄h)-国模网站-亚洲激情四射 | 东北熟妇大叫高潮91-gay片网站三级片无码-老师自慰毛茸茸-紧18成网站 | wwww啊啊啊啊-91肏你-蓝光电影在线看 亚洲欧美一二三区-老熟女翔田千里与黑人 | 美女裸网站国产-颤抖到了绝顶高潮合集-XXXXX潢色-国产老太婆乱子伦农村 | Chinese高潮潮喷叫床-亚洲色网淫色网-黑人操日本女人网站-欲婷婷影院 | 超清最新电影在线观看 蜻蜓点水服务是指什么意思-日日爱爱视频-亚洲Aⅴ日韩无码黄片-风间由美777久久久精品 | 午夜理伦精品一区二区三区在线成人-┅┅用力┅┅老熟女-国产精品三上悠亚在线观看网站-东北电影免费老师无码黄色片视屏网站大全 亚洲美女自慰-七十路熟女视频-日韩小穴-色女人综合 | jizzjizz日本熟妇-成熟美妇高潮欲仙欲死-肥臀熟女乱伦-国产熟女情人口爆正在播放 | 人妻交换第一区-无套中出大桥未久-中日韩一区二区视频-2019中文字幕日韩 | 少妇口述玌伦经过全文阅读-大奶骚影院-国产在线视频一区二区-强奸妞视频影视大全网站 | 五级片AV-久久久久久久人妻无码中文-五十路熟妇在线观看-日本无码熟妇风间由美 | 午夜一级剧厂-久热天色五月四虎-黄色人人插-熟女一二三王 | 北条麻纪女同-国产裸体老师无遮挡免费-在线精品自偷自拍无码白浆-一本正道久久熟女人妻 | 一道本日本欧美草草-免费观看国产不卡福利-有字幕完整版 国产熟妇无码A片AAA毛片视频-男人日女人人人网毛片 | 亚洲日韩欧美国产brandistep-中国老熟女重囗味hdxx-黑人泄欲一区二区三区-电影一区二区日韩电影 自拍偷拍视频43-黄片hhh-狠牛影视在线一区-久久精品视频4242 | 依依狼人日日-欧美顶级黃色大片免费-720高清视频播放 日本丰满熟妇人妻av无码区-亚洲三级黄色 三区无码 | free嫩白的16sex性自由-多毛熟女HD-JlZZJlZZ妇女亚洲人水多-在线观看一区二区国产日产英 | 国产精品18久久久久久不卡-日本wwwxxxx-49VV成人-迷j黑丝网站 | 538在线视频二区三区视视频-插妹子在线观看-久久成人亚洲香蕉草草是为大家提供多种视频资源的手机软件-日韩欧美中文在线精品 免费福利专区视频 | 淫熟交尾竹内纱里奈-长筒美女被操出白浆-性感小唯西川惊人的口交和性-日本xxxxxxx49 | freevido国产-导航色一二三三网-狼人大香蕉99-国产女主播精品大秀系列 | 韩国美女自慰视屏-一级片电影中文字幕-素人无码流出影视大全-久久狼人大香蕉 | 三个护士残忍榨精无码视频-国产亚洲午夜精品国产亚洲-大香蕉在线视频8-亚洲国产成人在线精品 | 四十路中出精品区-饭岛爱网站免费入口-老司机熟女网站-91精品免费久久久久久久久 | 国产按摩店三级毛片-JJZZJZZJZZ成熟人妻-大香蕉久久伊人网-日韩美女裸交 | BD国语免费观看韩国 4314 4834 ** 国产做受XXX黑人XXⅩ-中日韩一区二区三区四区电影-大桥未久黑人mibd445-欧美老太黑人性爱影院 中文不卡av中文字幕-女人自慰免费观看网站-中国女人花心毛片视频网站-美艳嫩模呻吟啪啪呻吟 | 777777777亚洲大胆妇女-狼人综合干网-国产精品77777竹菊影视-亚色九九九视频 | jizz自拍bbw-成人午夜视频在线观看网址-扒开美女JK 狂揉 漫画-欧美性猛交xxxx免费看久久久 | av一级嗯嗯啊-成人美女-级视频-四虎永久在线精品-久久情爱网站 | 日本成人X片免费看-大地资源第二页在线高清-空姐女优洗澡被操视频免费-肥臀成熟美妇在线播放 | 亚洲中久无码不卡永久在线观看-国产精品嫩草AV城中村-日韩欧美视频免费看-皇后颤抖双乳呻吟求欢 粗暴av-懂色AV粉嫩AV蜜乳AV-巨人黑人ⅴideos极品另类-太紧了中文字幕 | 久久久久-胸好大用力深一点-黄色xxxxxxxxxxxxll-极品色av影院 | 香蕉视频在线视频-97色情网-高清迅雷资源,在线手机播放-亚洲不卡无码av 中文字幕 | 摸BBB揉BBB揉BBB视频火-国产操逼啊啊啊-丰满少妇被猛烈进入高清播放-下面湿的网站 | 爽妇导航-北条麻妃潮喷-BD英语高清在线 亚洲天堂视频在线观看-自拍偷拍视频网址 | 1080全集在线观看 欧美人与性囗牲恔配-欧美sss一级二级-农村肥妇一级特黄大片-浓厚交体液丰满少妇 | wwwtubecom中国熟女-水野优香中文字幕一区二区-欧美专区在线第十一页-91牛成人欧美大片 |